CHIP REPAIR

 

       Allow time for videos to download before viewing, review written instructions while waiting for videos

 

             1      

CHIP REPAIRS

 

ROLL-ON REFINISHING

 

IMPORTANT: When rolling a tub use KF-43 filler for repairs.  It is fast hardening and easy to sand. KF-43 can NOT be used unless it is being covered with a pigmented coating.  KF-43 it is NOT color fast and will yellow if exposed to light.

 

     

1.Sand chipped area  

2.Mix KF-43 filler 

3.Add white cream hardener  

4.Fill chip 

5.Harden filler  6.Sand smooth

 

Chips require filling, sanding, then applying a second thin coat of filler to get a virtually perfect repair

 

KF-43

 

CHIP FILLER & WHITE CREAM HARDENER

 


2

 CHIP REPAIR SURFACE PREP

Use 80 grit paper to rough up area


3

REMOVED SANDING DUST

With Damp Tack Cloth


4

AREA BEING REPAIRED MUST BE HEATED WITH HEAT GUN

PRIOR TO APPLYING FILLER

Heating surface removes moisture and starts hardening filler from the back side of the repair.

PORCELAIN SURFACES: Touch heated area with (back side) of hand. When areas is uncomfortable warm to touch but NOT to hot to touch then apply catalyzed filler. 

FIBERGLASS SURFACES: Use less heat on fiberglass it burns easily.

ACRYLIC SURFACES: WARNING Use only KF-47 Acrylic Filler and do NOT use any heat on acrylic surfaces. If heated the filler will crack around the edges when it cools. 


5

 

KF-43 CHIP REPAIR FILLER (MIXING)

Use KF-43 White Filler & White Cream Hardener

IMPORTANT: Do NOT over catalyze filler

 


6

HEATING CHIP FILLER

FILLED AREA REQUIRES HEATING WITH HEAT GUN

FILLER MUST BE HARD BEFORE SANDING

With a metal object like a screw driver etc, tap on tub beside filler then tap on filler.

When both filler and tub sound the same the filler is hard and ready to sand. 

 


7

SANDING CHIP FILLER TO CONTOUR

Use 80 grit paper by hand or with and small rubber sanding block

 


8

 

SANDING CHIP FILLER SMOOTH

Use 120 grit paper by hand or with and small rubber sanding block

 


9

IMPORTANT:

CHIP REPAIR IS A TWO STEP PROCESS

 


10

EACH CHIP MUST BE FILLED AND SANDED TWICE (2) Times

 TO GET A PERFECTLY SMOOTH SURFACE


11

 

CHIP FILLER REQUIRES HEATING FILLED AREA WITH HEAT GUN

FILLER MUST BE HARD BEFORE SANDING


12

SANDING CHIP FILLER

"FINAL SANDING"

Use 120 grit paper by hand or with and small rubber sanding block

 


13

TACK CLOTH

DUST REMOVAL

Dust removal is essential

 


AFTER ALL REPAIRS ARE COMPLETED

PROCEED TO  ETCHING  or  WIPE-ON PRIMER

 

 Close Page