CHIP REPAIRS

 

When restoring TUB with the NO Spray System

 

IMPORTANT: When restoring a tub with the NO SPRAY system use KF-40 filler and clear hardener for repairs.  KF-40 is color fast. It will retain its finished color and NOT yellow. 

 

Do NOT use KF-43 filler on any area that will not be covered with a pigmented coating such as, on the tub bottom under the Slip-Grip bottom surface or tub mat etc. KF-43 it is NOT color fast and will yellow if exposed to light.

 

 

USE KF-40 FILLER

 

     

 

1.Sand chipped area  

2.Mix KF-40 filler & color 

3.Add clear hardener 

4.Fill chip 

5.Harden filler 

6.Sand smooth

Chips require filling, sanding, then applying a second thin coat of filler to get a virtually perfect repair

 

 

 

See color chart in written instructions

 

Tints are Super concentrated use minute amounts of tint in filler

Apply tiny amounts with tip end of a straightened, paper clip to get right amount and color

 


2

 CHIP REPAIRS SURFACE PREP

 


3

CHIP REPAIR FILLER (MIXING)

White & Pastel Colors

Use KF-40 White Filler & Clear Hardener

IMPORTANT: Use minute amounts of tints for fine tuning filler color

Just a speck of concentrated tint will make a lot of difference in a color

 


4

CHIP REPAIR FILLER (MIXING)

Deep Colors

Use KF-41 Neutral Color, Filler

IMPORTANT: Use no more that 10% tints for deep colors


5

AREA BEING REPAIRED MUST BE HEATED WITH HEAT GUN

PRIOR TO APPLYING FILLER

Heating surface removes moisture and starts hardening filler from the back side of the repair.

PORCELAIN SURFACES: Touch heated area with (back side) of hand. When areas is uncomfortable warm to touch but NOT to hot to touch then apply catalyzed filler. 

FIBERGLASS SURFACES: Use less heat on fiberglass it burns easily.

ACRYLIC SURFACES: WARNING Use only KF-47 Acrylic Filler and do NOT use any heat on acrylic surfaces. If heated the filler will crack around the edges when it cools. 


6

CHIP REPAIR FILLER APPLICATION


7

FILLED AREA REQUIRES HEATING WITH HEAT GUN

FILLER MUST BE HARD BEFORE SANDING

With a metal object like a screw driver etc, tapp on tub beside filler then tap on filler.

When both filler and tub sound the same the filler is hard and ready to sand. 


8

SANDING CHIP FILLER TO CONTOUR

Use 100 - 120 grit paper and small rubber sanding block


9

CHIP REPAIR IS A TWO STEP PROCESS

T-5 DETECTOR LIGHT

 

Turn off overhead lights and use T-1 Detector Light to detect imperfections in filled chip AFTER sanding.

Apply a second coat of filler and sand for a perfect repair.

Follow written Instructions closely


10

EACH CHIP MUST BE FILLED AND SANDED TWICE (2) Times

 TO GET A PERFECTLY SMOOTH SURFACE


11

 

CHIP FILLER REQUIRES HEATING FILLED AREA WITH HEAT GUN

FILLER MUST BE HARD BEFORE SANDING


12

SANDING CHIP FILLER

"FINAL SANDING"


13

TACK CLOTH

DUST REMOVAL

Dust removal is essential

 


14

2-W

COLOR BLENDING CHIP REPAIRS

Choose correct color 2-W blender

Different color 2-W can be placed on applicator pad to adjust color of repair

Apply 2-W to repaired area with applicator pad in a dabbing and wiping motion alternately

 


15

 

CHIP REPAIR,

FINAL TREATMENT WHEN USING 2-W

 


16

FINISHED REPAIR